Product family
HASTELLOY® W alloy
Made by Haynes International, INC
- Uts
- 112.9 ksi
- Yield
- 69.9 ksi
- Density
- 8.22 g/cm3
- Material
- Nickel-based superalloy
- Modulus rt
- 29.8 x10^6 psi
- Cte 79-200f
- 7.7 µin/in-°F
- Elong % 70f
- 48.9 %
- Poisson 72f
- 0.32
- Uts ksi 70f
- 340 ksi
- Cte 79-1000f
- 8.4 µin/in-°F
- Cte 79-1200f
- 8.6 µin/in-°F
- Cte 79-1350f
- 8.8 µin/in-°F
- Cte 79-1400f
- 8.9 µin/in-°F
- Cte 79-1500f
- 8.9 µin/in-°F
- Cte 79-1600f
- 9.1 µin/in-°F
- Cte 79-1650f
- 9.1 µin/in-°F
- Cte 79-1800f
- 9.2 µin/in-°F
- Modulus 200f
- 29.4 x10^6 psi
- Modulus 400f
- 28.6 x10^6 psi
- Modulus 600f
- 27.8 x10^6 psi
- Modulus 800f
- 26.7 x10^6 psi
- Elong % 1000f
- 60.2 %
- Elong % 1200f
- 63.5 %
- Elong % 1400f
- 74.5 %
- Elong % 1600f
- 98.1 %
- Elong % 1800f
- 98.1 %
- Elong % 2000f
- 95.3 %
- Melting range
- 1260-1355°C
- Modulus 1000f
- 25.8 x10^6 psi
- Modulus 1200f
- 24.7 x10^6 psi
- Modulus 1400f
- 23.3 x10^6 psi
- Modulus 1600f
- 22.2 x10^6 psi
- Modulus 1800f
- 20.4 x10^6 psi
- Poisson -108f
- 0.328
- Uts ksi 1000f
- 224 ksi
- Uts ksi 1200f
- 212 ksi
- Uts ksi 1400f
- 218 ksi
- Uts ksi 1600f
- 189 ksi
- Uts ksi 1800f
- 94 ksi
- Uts ksi 2000f
- 45 ksi
- Yield ksi 70f
- 49.3 ksi
- Resistivity 75f
- 45.21 µohm-in
- Yield ksi 1000f
- 32.5 ksi
- Yield ksi 1200f
- 30.7 ksi
- Yield ksi 1400f
- 31.6 ksi
- Yield ksi 1600f
- 27.4 ksi
- Yield ksi 1800f
- 13.6 ksi
- Yield ksi 2000f
- 6.5 ksi
- Resistivity 100f
- 45.38 µohm-in
- Resistivity 200f
- 45.89 µohm-in
- Resistivity 300f
- 46.31 µohm-in
- Resistivity 400f
- 46.78 µohm-in
- Resistivity 500f
- 47.20 µohm-in
- Resistivity 600f
- 47.53 µohm-in
- Resistivity 700f
- 47.93 µohm-in
- Resistivity 800f
- 48.23 µohm-in
- Resistivity 900f
- 48.61 µohm-in
- Specific heat rt
- 0.116 Btu/lb-°F
- Resistivity 1000f
- 49.00 µohm-in
- Resistivity 1100f
- 49.38 µohm-in
- Resistivity 1200f
- 49.53 µohm-in
- Resistivity 1300f
- 49.61 µohm-in
- Resistivity 1400f
- 49.68 µohm-in
- Resistivity 1500f
- 49.73 µohm-in
- Resistivity 1600f
- 49.80 µohm-in
- Resistivity 1700f
- 49.81 µohm-in
- Resistivity 1800f
- 49.67 µohm-in
- Resistivity 1900f
- 49.59 µohm-in
- Resistivity 2000f
- 49.57 µohm-in
- Specific heat 100c
- 486 J/kg-°C
- Specific heat 200c
- 487 J/kg-°C
- Specific heat 200f
- 0.117 Btu/lb-°F
- Specific heat 300c
- 484 J/kg-°C
- Specific heat 400c
- 491 J/kg-°C
- Specific heat 400f
- 0.118 Btu/lb-°F
- Specific heat 500c
- 507 J/kg-°C
- Specific heat 600c
- 531 J/kg-°C
- Specific heat 600f
- 0.119 Btu/lb-°F
- Specific heat 700c
- 564 J/kg-°C
- Specific heat 800c
- 606 J/kg-°C
- Specific heat 800f
- 0.123 Btu/lb-°F
- Specific heat 900c
- 657 J/kg-°C
- Specific heat 1000c
- 716 J/kg-°C
- Specific heat 1000f
- 0.130 Btu/lb-°F
- Specific heat 1100c
- 784 J/kg-°C
- Specific heat 1200f
- 0.139 Btu/lb-°F
- Specific heat 1400f
- 0.151 Btu/lb-°F
- Specific heat 1600f
- 0.167 Btu/lb-°F
- Specific heat 1800f
- 0.186 Btu/lb-°F
- Specific heat 2000f
- 0.205 Btu/lb-°F
- Thermal conductivity 70f
- 9.2 W/m-°C
- Thermal conductivity 200f
- 11.2 W/m-°C
- Thermal conductivity 500f
- 14.1 W/m-°C
- Thermal conductivity 1100f
- 20.9 W/m-°C
- Thermal conductivity 1200f
- 21.9 W/m-°C
- Thermal conductivity 1300f
- 22.8 W/m-°C
- Thermal conductivity 1400f
- 23.8 W/m-°C
- Thermal conductivity 1500f
- 24.7 W/m-°C
- Thermal conductivity 1600f
- 25.7 W/m-°C
- Thermal conductivity 1700f
- 26.7 W/m-°C
From Haynes International, INC’s own documents · read October 12, 2026 · not verified by FactoryRegistry
2 families in HASTELLOY® W alloy
Documents
Where this comes from — 2 documents
A machine read this from documents Haynes International, INC publishes on its own website, as of October 12, 2026. FactoryRegistry has not verified it; the documents are the authority.
- HASTELLOYWalloy, page 1: “HASTELLOY® W alloy (UNS N10004) is a solid-solution-strengthened super alloy”
- HASTELLOYWalloy: “HASTELLOYWalloy”
- HASTELLOYXalloy, page 5: “yield_ksi_70f: 49.3 ksi”